eFunda: Properties of Alloy Steel AISI 8630
engineering fundamentals Alloy Steel AISI 8630
Directory | Career | News | Standards | Industrial | SpecSearch®
Metal Alloys
Alloy Home
Steels
Alloy Steels
General Information
Properties
Classification
Standard
H-Steels
HSLA
Alloy Steel List
AISI 1xxx
AISI 2xxx
AISI 3xxx
AISI 4xxx
AISI 5xxx
AISI 6xxx
AISI 8xxx
AISI 9xxx
* For other AISI or Non-AISI, please use the search function above or check Grades.
ASTM Steels
Resources
Bibliography
Login

Home Membership Magazines Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
AISI 8630
Category Steel
Class Alloy steel
Type Standard
Common Names Nickel-chromium-molybdenum steel
Designations  Germany: DIN 1.6545
Italy: UNI 30 NiCrMo 2 KB
United States: AMS 6280 , AMS 6280E , AMS 6281 , AMS 6281C , AMS 6355 , AMS 6355G , AMS 6530 , AMS 6530E , AMS 6550 , AMS 6550E , ASTM A322 , ASTM A331 , ASTM A505 , ASTM A519 , MIL SPEC MIL-S-16974 , SAE J404 , SAE J412 , SAE J770 , UNS G86300

Composition

ElementWeight %
C  0.28-0.33 
Mn  0.70-0.90 
P  0.035 (max) 
S  0.04 (max) 
Si  0.15-0.30 
Cr  0.40-0.60 
Ni  0.40-0.70 
Mo  0.15-0.25 

Mechanical Properties

Properties Conditions 
T (°C)Treatment
Density (×1000 kg/m3) 7.7-8.03 25  
Poisson's Ratio 0.27-0.30 25  
Elastic Modulus (GPa) 190-210 25  
Tensile Strength (Mpa) 564.0  25  annealed at 845°C  more
Yield Strength (Mpa) 372.3 
Elongation (%) 29.0 
Reduction in Area (%) 58.9 
Hardness (HB) 156  25  annealed at 845°C more
Impact Strength (J)
(Izod)
95.2  25  annealed at 845°C  more

Thermal Properties

Properties Conditions 
T (°C)Treatment
Thermal Expansion (10-6/ºC) 11.2  21-100 more  