AISI 8650 |
 |
|
| Category | Steel |
| Class | Alloy steel |
| Type | Standard |
| Common Names | Nickel-chromium-molybdenum steel |
| Designations |
United States: ASTM A322 , ASTM A505 , ASTM A519 , SAE J404 , SAE J412 , SAE J770 , UNS G86500
|
| Composition |
 |
|
| Element | Weight % |
| C |
0.48-0.53 |
| Mn |
0.75-1.00 |
| P |
0.035 (max) |
| S |
0.04 (max) |
| Si |
0.15-0.30 |
| Cr |
0.40-0.60 |
| Ni |
0.40-0.70 |
| Mo |
0.15-0.25 |
|
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
7.7-8.03
|
25 |
|
| Poisson's Ratio |
0.27-0.30 |
25 |
|
| Elastic Modulus (GPa) |
190-210
|
25 |
|
| Tensile Strength (Mpa) |
715.7 |
25 |
annealed at 795°C more |
| Yield Strength (Mpa) |
386.1 |
| Elongation (%) |
22.5 |
| Reduction in Area (%) |
46.4 |
| Hardness (HB) |
212 |
25 |
annealed at 795°C more |
Impact Strength (J) (Izod) |
29.4 |
25 |
annealed at 795°C more |
|