eFunda: Properties of Copper Alloy UNS C61500
engineering fundamentals Copper Alloy UNS C61500
Directory | Career | News | Industrial
Metal Alloys
Alloy Home
Copper Alloys
General Information
Properties
Cu Alloy Types
Cast Alloys
Wrought Alloys
Cu Alloy List
UNS C1xxxx
UNS C2xxxx
UNS C3xxxx
UNS C4xxxx
UNS C5xxxx
UNS C6xxxx
UNS C7xxxx
UNS C8xxxx
UNS C9xxxx
Specific Cu Alloy
General Information
Resources
Bibliography
Login

Home Membership Magazines Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
UNS C61500
Category Copper Alloy
Class Wrought
Type Aluminum bronze
Designations United States: UNS C61500

Composition

ElementWeight %
Cu  90.0 
Al  8.0 
Ni  2.0 

Mechanical Properties

Properties Conditions 
T (°C)Treatment
Density (×1000 kg/m3) 8.8-8.94 25  
Poisson's Ratio 0.34 25  
Elastic Modulus (GPa) 117 25  
Tensile Strength (Mpa) 483-1000 25  (flat products) 
Yield Strength (Mpa) 152-965
Elongation (%) 55 
Reduction in Area (%)  
Note: Elongation is measured in 1 inch.