UNS C90300 |
 |
|
| Category | Copper Alloy |
| Class | Cast |
| Type | Tin bronze |
| Designations | United States: UNS C90300, ASTM B584 |
| Composition |
 |
|
| Element | Weight % |
| Cu |
88 |
| Sn |
8 |
| Zn |
4 |
|
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
8.8-8.94
|
25 |
|
| Poisson's Ratio |
0.34 |
25 |
|
| Elastic Modulus (GPa) |
117
|
25 |
|
| Tensile Strength (Mpa) |
310 |
25 |
(castings: centrifugal, continuous, investment, plaster, sand) |
| Yield Strength (Mpa) |
145 |
| Elongation (%) |
30 |
| Reduction in Area (%) |
|
| Hardness (HB500) |
70 |
25 |
(as cast) |
|