AISI 5160H |
 |
|
| Category | Steel |
| Class | Alloy steel |
| Type | H-steel |
| Common Names | Chromium steel |
| Designations |
United States: ASTM A304 , SAE J1268 , UNS H51600
|
| Composition |
 |
|
| Element | Weight % |
| C |
0.55-0.65 |
| Mn |
0.65-1.10 |
| Cr |
0.60-1.00 |
| P |
0.035 |
| S |
0.040 |
| Si |
0.15-0.30 |
|
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
7.7-8.03
|
25 |
|
| Poisson's Ratio |
0.27-0.30 |
25 |
|
| Elastic Modulus (GPa) |
190-210
|
25 |
|
| Tensile Strength (Mpa) |
724 |
25 |
annealed at 815°C more |
| Yield Strength (Mpa) |
275 |
| Elongation (%) |
17.2 |
| Reduction in Area (%) |
31 |
| Hardness (HB) |
197 |
25 |
annealed at 815°C more |
|