Ti-6Al-4V-ELI (low O2) |
 |
|
| Category | Titanium Alloy |
| Class | Wrought |
| Type | Alpha-beta alloy |
| Designations | United States: MIL-T-9046, MIL-T-9047, AMS 4930, AMS 4907, AMS 4956 |
| Composition |
 |
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
4.43 |
25 |
|
| Poisson's Ratio |
0.34200001 |
25 |
|
| Elastic Modulus (GPa) |
113.8 |
25 |
|
| Tensile Strength (Mpa) |
896 |
25 |
annealed |
| Yield Strength (Mpa) |
827 |
| Elongation (%) |
15 |
| Reduction in Area (%) |
35 |
| Hardness (HRC) |
35 |
25 |
annealed |
Impact Strength (J) (Charpy) |
24 |
25 |
annealed |
| Thermal Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Thermal Expansion (10-6/ºC) |
8.6 |
20-100 more |
|
|