99.1 Ti |
 |
|
| Category | Titanium Alloy |
| Class | Wrought |
| Type | Commercially Pure |
| Designations | United States: ASTM B265 Grade3, ASTM B348 Grade3, ASTM B381 Grade3, MIL-T-9046, ,AMS 4900 |
| Composition |
 |
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
4.51 |
25 |
|
| Poisson's Ratio |
0.34 |
25 |
|
| Elastic Modulus (GPa) |
103.4 |
25 |
|
| Tensile Strength (Mpa) |
234 |
315 more |
annealed |
| Yield Strength (Mpa) |
138 |
| Elongation (%) |
34 |
| Reduction in Area (%) |
75 |
| Hardness (HB) |
225 |
25 |
annealed |
Impact Strength (J) (Charpy) |
38 |
25 |
annealed |
| Thermal Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Thermal Expansion (10-6/ºC) |
8.6 |
20-100 more |
|
|