Ti-5Al-2.5Sn |
 |
|
| Category | Titanium Alloy |
| Class | Wrought |
| Type | Alpha alloy |
| Designations | United States: ASTM B265 Grade6, ASTM B348 Grade6, ASTM B381 Grade6, MIL-T-9046, MIL-T-9047, AMS 4926, AMS 4910, AMS 4966, AMS 4953 |
| Composition |
 |
|
| Element | Weight % |
| Al |
5 |
| Sn |
2.5 |
|
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
4.48 |
25 |
|
| Poisson's Ratio |
0.33 |
25 |
|
| Elastic Modulus (GPa) |
110.3 |
25 |
|
| Tensile Strength (Mpa) |
565 |
315 more |
annealed |
| Yield Strength (Mpa) |
448 |
| Elongation (%) |
18 |
| Reduction in Area (%) |
45 |
| Hardness (HRC) |
36 |
25 |
annealed |
Impact Strength (J) (Charpy) |
26 |
25 |
annealed |
| Thermal Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Thermal Expansion (10-6/ºC) |
9.4 |
20-100 more |
|
|