eFunda Polymers: Properties of Polyamide {nylon (PA 6), 30% glass fiber reinforced, impact modified}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyamide
 
List of Suppliers
State: nylon (PA 6)
Additives: 30% glass fiber reinforced, impact modified
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   8418  tensile  dry (0.2% water content) D638
  5203  tensile  50% relative humidity D638
Flexural Modulus (MPa)   8004   23 ºC  dry (0.2% water content) D790
  4140   23 ºC  50% relative humidity D790
Tensile Strength (MPa)  101 at break  50% relative humidity D638
 145 at break  dry (0.2% water content) D638
Elongation at break (%)   5    dry (0.2% water content) D638
  8    50% relative humidity D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  3.2    50% relative humidity D256A
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  1.2    dry (0.2% water content) D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   20 - 25     D696
Deflection Temperature (ºC)  220   0.46 MPa  dry (0.2% water content) D648
 210   1.82 MPa  dry (0.2% water content) D648

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.33   D792
Water Absorption (% weight increase)  6.2  saturated D570
 2  after 24 hrs D570

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  220  Tm, crystalline  
Processing Temperature (ºC)  249 - 288  injection molding  
Molding Pressure (MPa)   21 - 138    
Compression Ratio  3 - 4    
Linear Mold Shrinkage (cm/cm)  0.003 - 0.005   D955

Top of Page

Suppliers
Adell Plastics, Inc. Baltimore, MD  800-638-5218
Albis Corp. Rosenburg, TX  800-231-5911
AlliedSignal, Inc. Morristown, NJ  888-565-9835
Ashley Polymers Brooklyn, NY   
Bamberger Polymers, Inc. Jericho, NY   
BASF Corp. Mount Olive, NJ  800-BC-RESIN
Bayer Corp. Pittsburgh, PA  800-662-2927
ComAlloy International Co. Nashville, TN   
EMS-American Grilon, Inc. Sumter, SC   
Ferro Corp. Cleveland, OH   
LNP Engineering Plastics, Inc. Exton, PA  800-854-8774
M.A. Hanna Engineered Materials Norcross, GA   
M.A. Industries, Inc. Peachtree City, GA  800-241-8250
Network Polymers, Inc. Akron, OH  888-437-4674
Polymers International, Inc. Spartanburg, SC   
RTP Co. Winona, MN  800-433-4787

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.