eFunda Polymers: Properties of Polyamide {nylon (PA 66), 30-33% glass fiber reinforced}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyamide
 
List of Suppliers
State: nylon (PA 66)
Additives: 30-33% glass fiber reinforced
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   9522  tensile  dry (0.2% water content) D638
  7521  tensile  50% relative humidity D638
Flexural Modulus (MPa)   8280 - 10005   23 ºC  dry (0.2% water content) D790
  5520   23 ºC  50% relative humidity D790
  6210   23 ºC   D790
Tensile Strength (MPa)  191 at break  dry (0.2% water content) D638
 141 at break  50% relative humidity D638
 173 at yield  dry (0.2% water content) D638
Compressive Strength (MPa)
at yield or break
 166 - 276     D695
Flexural Strength (MPa)
at yield or break
 276  dry (0.2% water content)   D790
Flexural Strength (MPa)
at yield or break
 201  50% relative humidity   D790
Elongation at break (%)   2 - 4    dry (0.2% water content) D638
  3 - 7    50% relative humidity D638
Hardness  101 - 119  Rockwell R  dry (0.2% water content) D638
 101 - 102  Rockwell M  dry (0.2% water content) D638
  96  Rockwell M  50% relative humidity D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.8 - 2.4    dry (0.2% water content) D256A
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  1.4 - 1.6    50% relative humidity D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   15 - 54     D696
Deflection Temperature (ºC)  127 - 260   0.46 MPa  dry (0.2% water content) D648
 123 - 255   1.82 MPa  dry (0.2% water content) D648
Thermal Conductivity (W/m-ºC)  0.213 - 0.489     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.15 - 1.4   D792
Water Absorption (% weight increase)  5.5 - 6.5  saturated D570
 0.7 - 1.1  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  360 - 500   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  260 - 265  Tm, crystalline  
Processing Temperature (ºC)  266 - 305  injection molding  
Molding Pressure (MPa)   35 - 138    
Compression Ratio  3 - 4    
Linear Mold Shrinkage (cm/cm)  0.002 - 0.006   D955

Top of Page

Suppliers
A. Schulman Akron, OH  800-662-7203
Adell Plastics, Inc. Baltimore, MD  800-638-5218
Albis Corp. Rosenburg, TX  800-231-5911
ALM Corp. Wayne, NJ   
Ashley Polymers Brooklyn, NY   
Bamberger Polymers, Inc. Jericho, NY   
BASF Corp. Mount Olive, NJ  800-BC-RESIN
Bayer Corp. Pittsburgh, PA  800-662-2927
ComAlloy International Co. Nashville, TN   
DSM Engineering Plastic Products, Inc. Reading, PA  800-729-0101
DuPont Co., Polymers Wilmington, DE  800-438-7225
EMS-American Grilon, Inc. Sumter, SC   
Ferro Corp. Cleveland, OH   
LNP Engineering Plastics, Inc. Exton, PA  800-854-8774
M.A. Hanna Engineered Materials Norcross, GA   
MRC Polymers, Inc. Chicago, IL   
Network Polymers, Inc. Akron, OH  888-437-4674
Nyltech NA Co., Inc. Manchester, NH   
Polymer Resources, Ltd. Farmington, CT  800-243-5176
Polymers International, Inc. Spartanburg, SC   
RTP Co. Winona, MN  800-433-4787
Solutia, Inc. St Louis, MO   
Thermofil, Inc. Brighton, MI  800-444-4408
Ticona Summit, NJ  800-526-4960
Wellman, Inc. Johnsonville, SC   