eFunda Polymers: Properties of Polyamide {nylon (PA 6), 15% glass fiber reinforced}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyamide
 
List of Suppliers
State: nylon (PA 6)
Additives: 15% glass fiber reinforced
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   5507  tensile  dry (0.2% water content) D638
  3506  tensile  50% relative humidity D638
Flexural Modulus (MPa)   4830   23 ºC  dry (0.2% water content) D790
  2898   23 ºC  50% relative humidity D790
Tensile Strength (MPa)  131 at break  dry (0.2% water content) D638
  71 at break  50% relative humidity D638
Elongation at break (%)   4    dry (0.2% water content) D638
  6    50% relative humidity D638
Hardness   92  Rockwell M  dry (0.2% water content) D638
  74  Rockwell M  50% relative humidity D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.6     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   52     D696
Deflection Temperature (ºC)  215   0.46 MPa   D648
 190   1.82 MPa   D648

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.23   D792
Water Absorption (% weight increase)  8  saturated D570
 2.6  after 24 hrs D570

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  220  Tm, crystalline  
Processing Temperature (ºC)  272 - 291  general  
Linear Mold Shrinkage (cm/cm)  0.002 - 0.003   D955

Top of Page

Suppliers
A. Schulman Akron, OH  800-662-7203
Ashley Polymers Brooklyn, NY   
BASF Corp. Mount Olive, NJ  800-BC-RESIN
Bayer Corp. Pittsburgh, PA  800-662-2927
ComAlloy International Co. Nashville, TN   
EMS-American Grilon, Inc. Sumter, SC   
M.A. Hanna Engineered Materials Norcross, GA   
M.A. Industries, Inc. Peachtree City, GA  800-241-8250
Network Polymers, Inc. Akron, OH  888-437-4674
Nyltech NA Co., Inc. Manchester, NH   
Polymers International, Inc. Spartanburg, SC   
RTP Co. Winona, MN  800-433-4787
Wellman, Inc. Johnsonville, SC   

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.