eFunda Polymers: Properties of Polyethylene and ethylene copolymers {high density, 30% glass fiber reinforced}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyethylene and ethylene copolymers
 
List of Suppliers
State: high density
Additives: 30% glass fiber reinforced
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   4830 - 6210  tensile   D638
Flexural Modulus (MPa)   4830 - 5520   23 ºC   D790
Tensile Strength (MPa)   52 - 63 at break   D638
Compressive Strength (MPa)
at yield or break
  42 - 49     D695
Flexural Strength (MPa)
at yield or break
  76 - 83     D790
Elongation at break (%)   2 - 3     D638
Hardness   75 - 90  Rockwell R   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.6 - 0.8     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   48     D696
Deflection Temperature (ºC)  127 - 130   0.46 MPa   D648
 122   1.82 MPa   D648
Thermal Conductivity (W/m-ºC)  0.359 - 0.460     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.18 - 1.28   D792
Water Absorption (% weight increase)  0.02 - 0.06  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  500 - 550   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  120 - 140  Tm, crystalline  
Processing Temperature (ºC)  177 - 316  injection molding  
Molding Pressure (MPa)   69 - 138    
Linear Mold Shrinkage (cm/cm)  0.002 - 0.006   D955

Top of Page

Suppliers
A. Schulman Akron, OH  800-662-7203
ComAlloy International Co. Nashville, TN   
DSM Engineering Plastic Products, Inc. Reading, PA  800-729-0101
Ferro Corp. Cleveland, OH   
LNP Engineering Plastics, Inc. Exton, PA  800-854-8774
M.A. Industries, Inc. Peachtree City, GA  800-241-8250
RTP Co. Winona, MN  800-433-4787
Thermofil, Inc. Brighton, MI  800-444-4408

Top of Page