eFunda Polymers: Properties of Polyethylene and ethylene copolymers {high density copolymer, low and medium molecular weight}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyethylene and ethylene copolymers
 
List of Suppliers
State: high density copolymer, low and medium molecular weight
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   621 - 897  tensile   D638
Flexural Modulus (MPa)   828 - 1242   23 ºC   D790
Tensile Strength (MPa)   21 - 45 at break   D638
  18 - 29 at yield   D638
Compressive Strength (MPa)
at yield or break
  19 - 25     D695
Elongation at break (%)   10 - 1300     D638
Hardness   58 - 70  Shore D   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.2 - 3.2     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   70 - 110     D696
Deflection Temperature (ºC)   65 - 80   0.46 MPa   D648
Thermal Conductivity (W/m-ºC)  0.418     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  0.939 - 0.96   D792
Water Absorption (% weight increase)  0 - 0.01  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  450 - 500   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  125 - 132  Tm, crystalline  
Processing Temperature (ºC)  191 - 260  injection molding  
 149 - 260  extrusion  
Molding Pressure (MPa)   35 - 138    
Compression Ratio  2    
Linear Mold Shrinkage (cm/cm)  0.012 - 0.04   D955

Top of Page

Suppliers
A. Schulman Akron, OH  800-662-7203
AlphaGary Corp. Leominster, MA  800-232-9741
American Polymers, Inc. Worcester, MA   
Bamberger Polymers, Inc. Jericho, NY   
Chevron Chemical Co. Houston, TX  800-231-3828
Dow Plastics Midland, MI  800-441-4369
Eastman Chemical Co. Kingsport, TN  800-327-8626
Equistar Chemicals LP Houston, TX  888-777-0232
Exxon Chemical Canada Toronto, Ontario, M5W 1K3, Canada   
Exxon Chemical Co. Houston, TX  800-231-6633
Fina Oil & Chemical Co. Dallas, TX  800-344-3462
Mobil Chemical Co. Edison, NJ   
Network Polymers, Inc. Akron, OH  888-437-4674
NOVA Chemicals, Ltd. Calgary, Alberta T2P 5C6, Canada   
Phillips Chemical Co. Bartlesville, OK  800-537-3746
R.S.G. Polymers Corp. Stony Brook, NY   
Shuman Plastics, Inc. Depew, NY   
Ticona Summit, NJ  800-526-4960
Union Carbide Corp. Danbury, CT  800-335-8550

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.