eFunda Polymers: Properties of Polyimide {thermoset, unfilled}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyimide
 
List of Suppliers
State: thermoset
Additives: unfilled
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   3174 - 32085  tensile   D638
  2905  compressive   D638
Flexural Modulus (MPa)   2912 - 20700   23 ºC   D790
  7107 - 18561  149 ºC   D790
Tensile Strength (MPa)   30 - 159 at break   D638
  30 - 159 at yield   D638
Compressive Strength (MPa)
at yield or break
 134 - 228     D695
Flexural Strength (MPa)
at yield or break
  45 - 345     D790
Elongation at break (%)   1     D638
Hardness  110 - 120  Rockwell M   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.3 - 8.0     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   15 - 50     D696
Deflection Temperature (ºC)  300 - 302   1.82 MPa   D648
Thermal Conductivity (W/m-ºC)  0.230 - 0.502     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.41 - 1.9   D792
Water Absorption (% weight increase)  0.45 - 1.25  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  480 - 508   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  thermoset  Tm, crystalline  
Processing Temperature (ºC)  238 - 252  general  
Molding Pressure (MPa)   49 - 200    
Compression Ratio  1 - 1.2    
Linear Mold Shrinkage (cm/cm)  0.001 - 0.01   D955

Top of Page

Suppliers
Ciba Specialty Chemicals Corp. Tarrytown, NY  800-431-2360

Top of Page