eFunda Polymers: Properties of Polypropylene {homopolymer, unfilled}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polypropylene
 
List of Suppliers
State: homopolymer
Additives: unfilled
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   1139 - 1553  tensile   D638
  1035 - 2070  compressive   D638
Flexural Modulus (MPa)   1173 - 1725   23 ºC   D790
  345   94 ºC   D790
  242  122 ºC   D790
Tensile Strength (MPa)   32 - 42 at break   D638
  32 - 38 at yield   D638
Compressive Strength (MPa)
at yield or break
  38 - 56     D695
Flexural Strength (MPa)
at yield or break
  42 - 56     D790
Elongation at break (%)   100 - 600     D638
Hardness   80 - 102  Rockwell R   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.2 - 0.7     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   81 - 100     D696
Deflection Temperature (ºC)  108 - 122   0.46 MPa   D648
  49 - 60   1.82 MPa   D648
Thermal Conductivity (W/m-ºC)  0.117     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  0.9 - 0.91   D792
Water Absorption (% weight increase)  0.01 - 0.03  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  600   D149

 Processing Properties Conditions
Type ASTM
Melt Flow (gm/10 min)  0.4 - 100   D1238
Melting Temperature (ºC)   -20  Tg, amorphous  
Melting Temperature (ºC)  160 - 175  Tm, crystalline  
Processing Temperature (ºC)  191 - 288  injection molding  
 205 - 260  extrusion  
Molding Pressure (MPa)   69 - 138    
Compression Ratio  2 - 2.4    
Linear Mold Shrinkage (cm/cm)  0.01 - 0.025   D955

Top of Page

Suppliers
A. Schulman Akron, OH  800-662-7203
American Polymers, Inc. Worcester, MA   
Amoco Chemicals Lisle, IL  800-621-4567
Aristech Chemical Corp. Pittsburgh, PA   
Bamberger Polymers, Inc. Jericho, NY   
ComAlloy International Co. Nashville, TN   
Dow Plastics Midland, MI  800-441-4369
Epsilon Products Co. Marcus Hook, PA  800-522-7509
Equistar Chemicals LP Houston, TX  888-777-0232
Exxon Chemical Co. Houston, TX  800-231-6633
Federal Plastics Corp. Cranford, NJ  800-541-4424
Ferro Corp. Cleveland, OH   
Fina Oil & Chemical Co. Dallas, TX  800-344-3462
Huntsman Corp. Salt Lake City, UT  800-421-2411
Montell North America Wilmington, DE   
Network Polymers, Inc. Akron, OH  888-437-4674
Phillips Chemical Co. Bartlesville, OK  800-537-3746
R.S.G. Polymers Corp. Stony Brook, NY   
Shuman Plastics, Inc. Depew, NY   
Solvay Polymers, Inc. Houston, TX  800-231-6313