eFunda Polymers: Properties of Polyphenylene Sulfide {unfilled}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyphenylene Sulfide
 
List of Suppliers
Additives: unfilled
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   3312  tensile   D638
Flexural Modulus (MPa)   3795 - 4140   23 ºC   D790
Tensile Strength (MPa)   49 - 87 at break   D638
Compressive Strength (MPa)
at yield or break
 111     D695
Flexural Strength (MPa)
at yield or break
  97 - 145     D790
Elongation at break (%)   1 - 6     D638
Hardness  123 - 125  Rockwell R   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.3     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   27 - 49     D696
Deflection Temperature (ºC)  199   0.46 MPa   D648
 100 - 135   1.82 MPa   D648
Thermal Conductivity (W/m-ºC)  0.084 - 0.288     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.35   D792
Water Absorption (% weight increase)  0.01 - 0.07  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  380 - 450   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)   88  Tg, amorphous  
Melting Temperature (ºC)  285 - 290  Tm, crystalline  
Processing Temperature (ºC)  310 - 338  injection molding  
Molding Pressure (MPa)   35 - 104    
Compression Ratio  2 - 3    
Linear Mold Shrinkage (cm/cm)  0.006 - 0.014   D955

Top of Page

Suppliers
Phillips Chemical Co. Bartlesville, OK  800-537-3746
Ticona Summit, NJ  800-526-4960

Top of Page