eFunda Polymers: Properties of Vinyl polymers and copolymers {PVC and PVC-AMC, tin-stabilized, sheets, rods and tubes; rigid}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Vinyl polymers and copolymers
 
List of Suppliers
State: PVC and PVC-AMC
Additives: tin-stabilized
Application: sheets, rods and tubes; rigid
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   2139 - 3002  tensile   D638
Flexural Modulus (MPa)   2105 - 2898   23 ºC   D790
Tensile Strength (MPa)   36 - 53 at yield   D638
Flexural Strength (MPa)
at yield or break
  44 - 94     D790
Hardness   69 - 78  Shore D   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  1.1 - 10.6     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   1 - 19     D696
Deflection Temperature (ºC)   72 - 75   0.46 MPa   D648
  21 - 73   1.82 MPa   D648

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.32 - 1.45   D792

 Processing Properties Conditions
Type ASTM
Processing Temperature (ºC)  194 - 205  injection molding  
Compression Ratio  2    

Top of Page

Suppliers
AlphaGary Corp. Leominster, MA  800-232-9741
Colorite Plastic Co. Ridgefield, NJ  800-631-1577
CONDEA Vista Co. Houston, TX  800-841-4877
Georgia Gulf Corp. Atlanta, GA   
Keysor-Century Corp. Santa Clarita, CA  888-539-7671
Occidental Chemical Corp. Dallas, TX  800-578-8880
Rimtec Corp. Burlington, NJ  800-272-0069
Shintech Inc. Houston, TX   
Synergistic Polymer Systems, Inc. Bellaire, TX   

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.