eFunda Polymers: Properties of Acrylic {cast sheet}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Acrylic
 
List of Suppliers
Application: cast sheet
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   2691 - 3278  compressive   D638
  2139 - 21390  tensile   D638
Flexural Modulus (MPa)   2208 - 22149   23 ºC   D790
Tensile Strength (MPa)   46 - 76 at break   D638
Compressive Strength (MPa)
at yield or break
  76 - 132     D695
Flexural Strength (MPa)
at yield or break
  83 - 118     D790
Elongation at break (%)   2 - 7     D638
Hardness   80 - 102  Rockwell M   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.2 - 0.2     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   50 - 90     D696
Deflection Temperature (ºC)   74 - 113   0.46 MPa   D648
  37 - 102   1.82 MPa   D648
Thermal Conductivity (W/m-ºC)  0.167 - 0.251     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.17 - 1.2   D792
Water Absorption (% weight increase)  0.2 - 0.4  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  450 - 550   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)   90 - 105  Tg, amorphous  
Linear Mold Shrinkage (cm/cm)  0.0017   D955

Top of Page

Suppliers
Aristech Chemical Corp. Pittsburgh, PA   
AtoHaas Americas, Inc. Philadelphia, PA   
Cyro Industries Rockaway, NJ  800-631-5384
DuPont Co., Polymers Wilmington, DE  800-438-7225
ICI Acrylics, Inc. Cordova, TN  800-325-9577

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.