17-7PH |
 |
|
| Conditions | Tensile Properties |
| T (°C) | Treatment |
| 25 |
CH900 (plate, sheet, strip) |
Tensile Strength (MPa) |
1650 |
| Yield Strength (MPa) |
1590 |
| Elongation (%) |
1 |
| Reduction in Area (%) |
|
| 25 |
cold rolled (condition C) (plate, sheet, strip) |
Tensile Strength (MPa) |
1380 |
| Yield Strength (MPa) |
1210 |
| Elongation (%) |
1 |
| Reduction in Area (%) |
|
| 25 |
RH950 (bar) |
Tensile Strength (MPa) |
1275 |
| Yield Strength (MPa) |
1030 |
| Elongation (%) |
6 |
| Reduction in Area (%) |
10 |
| 25 |
RH950 (plate, sheet, strip) |
Tensile Strength (MPa) |
1450 |
| Yield Strength (MPa) |
1310 |
| Elongation (%) |
4 |
| Reduction in Area (%) |
|
| 25 |
TH1050 (bar) |
Tensile Strength (MPa) |
1170 |
| Yield Strength (MPa) |
965 |
| Elongation (%) |
6 |
| Reduction in Area (%) |
25 |
| 25 |
TH1050 (plate, sheet, strip) |
Tensile Strength (MPa) |
1240 |
| Yield Strength (MPa) |
1030 |
| Elongation (%) |
5 |
| Reduction in Area (%) |
|
|