eFunda: Properties of Alloy Steel Alloy Steel Alloy Steel Alloy Steel AISI 6150
engineering fundamentals Alloy Steel Alloy Steel Alloy Steel Alloy Steel AISI 6150
Directory | Career | News | Standards | Industrial | SpecSearch®
 
 
Metal Alloys
Alloy Home
Steels
Alloy Steels
General Information
Properties
Classification
Standard
H-Steels
HSLA
Alloy Steel List
AISI 1xxx
AISI 2xxx
AISI 3xxx
AISI 4xxx
AISI 5xxx
AISI 6xxx
AISI 8xxx
AISI 9xxx
* For other AISI or Non-AISI, please use the search function above or check Grades.
ASTM Steels
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
AISI 6150
ConditionsHardness
T (°C)TreatmentMethodValue
25 annealed at 815°C   HB 197 
25 normalized at 870°C   HB 269 
25 oil quenched, fine grained, tempered at 205°C   HB 538 
25 oil quenched, fine grained, tempered at 315°C   HB 483 
25 oil quenched, fine grained, tempered at 425°C   HB 420 
25 oil quenched, fine grained, tempered at 540°C   HB 345 
25 oil quenched, fine grained, tempered at 650°C   HB 282 