eFunda: Properties of Alloy Steel Alloy Steel Alloy Steel AISI 81B45
engineering fundamentals Alloy Steel Alloy Steel Alloy Steel AISI 81B45
Directory | Career | News | Standards | Industrial | SpecSearch®
 
 
Metal Alloys
Alloy Home
Steels
Alloy Steels
General Information
Properties
Classification
Standard
H-Steels
HSLA
Alloy Steel List
AISI 1xxx
AISI 2xxx
AISI 3xxx
AISI 4xxx
AISI 5xxx
AISI 6xxx
AISI 8xxx
AISI 9xxx
* For other AISI or Non-AISI, please use the search function above or check Grades.
ASTM Steels
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
AISI 81B45
Conditions Tensile Properties 
T (°C)Treatment
25 oil quenched, fine grained, tempered at 205°C   Tensile Strength (MPa) 2034 
Yield Strength (MPa) 1724 
Elongation (%) 10 
Reduction in Area (%) 33 
25 oil quenched, fine grained, tempered at 315°C   Tensile Strength (MPa) 1765 
Yield Strength (MPa) 1572 
Elongation (%)
Reduction in Area (%) 42 
25 oil quenched, fine grained, tempered at 425°C   Tensile Strength (MPa) 1407 
Yield Strength (MPa) 1310 
Elongation (%) 11 
Reduction in Area (%) 48 
25 oil quenched, fine grained, tempered at 540°C   Tensile Strength (MPa) 1103 
Yield Strength (MPa) 1027 
Elongation (%) 16 
Reduction in Area (%) 53 
25 oil quenched, fine grained, tempered at 650°C   Tensile Strength (MPa) 896 
Yield Strength (MPa) 793 
Elongation (%) 20 
Reduction in Area (%) 55 