AA 5182 |
 |
|
| Category | Aluminum Alloy |
| Class | Wrought |
| Composition |
 |
|
| Element | Weight % |
| Al |
95.2 |
| Mn |
0.35 |
| Mg |
4.5 |
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
2.6-2.8
|
25 |
|
| Poisson's Ratio |
0.33 |
25 |
|
| Elastic Modulus (GPa) |
70-80
|
25 |
|
| Tensile Strength (Mpa) |
420 |
25 |
H19 more |
| Yield Strength (Mpa) |
395 |
| Elongation (%) |
4 |
| Reduction in Area (%) |
|
| Hardness (HB500) |
58 |
25 |
O |
| Shear Strength (MPa) |
150 |
25 |
O |
| Fatigue Strength (MPa) |
140 |
25 |
O |
| Thermal Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Thermal Conductivity (W/m-K) |
123 |
25 |
All |
| Electric Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Electric Resistivity (10-9W-m) |
56 |
25 |
All |
|