AISI 1005 |
 |
|
| Category | Steel |
| Class | Carbon steel |
| Type | Standard |
| Designations |
United States: ASTM A29 , ASTM A510 , MIL SPEC MIL-S-11310 (CS1005) , SAE J403 , SAE J412 , UNS G10050
|
| Composition |
 |
|
| Element | Weight % |
| C |
0.06 (max) |
| Mn |
0.35 (max) |
| P |
0.04 (max) |
| S |
0.05 (max) |
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
7.872 |
25 |
|
| Poisson's Ratio |
0.27-0.30 |
25 |
|
| Elastic Modulus (GPa) |
190-210
|
25 |
|
| Thermal Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Thermal Expansion (10-6/ºC) |
12.6 |
0-100 more |
|
| Specific Heat (J/kg-K) |
481 |
50-100 more |
|
|