AISI 1055 |
 |
|
| Category | Steel |
| Class | Carbon steel |
| Type | Standard |
| Designations |
Germany: DIN 1.1209 United States: ASTM A29 , ASTM A510 , ASTM A576 , ASTM A682 , FED QQ-S-700 (1055) , SAE J403 , SAE J412 , SAE J414 , UNS G10550
|
| Composition |
 |
|
| Element | Weight % |
| C |
0.50-0.60 |
| Mn |
0.60-0.90 |
| P |
0.04 (max) |
| S |
0.05 (max) |
|
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
7.7-8.03
|
25 |
|
| Poisson's Ratio |
0.27-0.30 |
25 |
|
| Elastic Modulus (GPa) |
190-210
|
25 |
|
| Tensile Strength (Mpa) |
660 |
25 |
cold drawn (round bar (19-32 mm)) more |
| Yield Strength (Mpa) |
560 |
| Elongation (%) |
10 |
| Reduction in Area (%) |
40 |
| Hardness (HB) |
197 |
25 |
cold drawn (round bar (19-32 mm)) more |
| Thermal Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Thermal Expansion (10-6/ºC) |
14.8 |
20-700 more |
annealed |
|