eFunda: Properties of Carbon Steel Carbon Steel Carbon Steel AISI 1055
engineering fundamentals Carbon Steel Carbon Steel Carbon Steel AISI 1055
Directory | Career | News | Standards | Industrial | SpecSearch®
 
 
Metal Alloys
Alloy Home
Steels
Carbon Steels
General Information
Properties
Classification
Low-Carbon
Medium-Carbon
High-Carbon
Other Grades
Resulfurized
High-Mn
H-Steels
Carbon Steel List
AISI 10xx
AISI 11xx
AISI 12xx
AISI 15xx
ASTM Steels
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
AISI 1055
Conditions Tensile Properties 
T (°C)Treatment
25 cold drawn (round bar (19-32 mm))  Tensile Strength (MPa) 660 
Yield Strength (MPa) 560 
Elongation (%) 10 
Reduction in Area (%) 40 
25 hot rolled (round bar (19-32 mm))  Tensile Strength (MPa) 650 
Yield Strength (MPa) 355 
Elongation (%) 12 
Reduction in Area (%) 30 