eFunda: Properties of Carbon Steel AISI 1070
engineering fundamentals Carbon Steel AISI 1070
Directory | Career | News | Standards | Industrial | SpecSearch®
 
 
Metal Alloys
Alloy Home
Steels
Carbon Steels
General Information
Properties
Classification
Low-Carbon
Medium-Carbon
High-Carbon
Other Grades
Resulfurized
High-Mn
H-Steels
Carbon Steel List
AISI 10xx
AISI 11xx
AISI 12xx
AISI 15xx
ASTM Steels
Specific Carbon Stl.
General Information
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
AISI 1070
Category Steel
Class Carbon steel
Type Standard
Designations  France: AFNOR XC 68
Germany: DIN 1.1231
Sweden: SS 1770 , SS 1778
United States: AMS 5115 , AMS 5115C , ASTM A29 , ASTM A510 , ASTM A576 , ASTM A682 , MIL SPEC MIL-S-11713 (2) , SAE J403 , SAE J412 , SAE J414 , UNS G10700

Composition
ElementWeight %
C  0.65-0.75 
Mn  0.60-0.90 
P  0.04 (max) 
S  0.05 (max) 

Mechanical Properties
Properties Conditions 
T (°C)Treatment
Density (×1000 kg/m3) 7.7-8.03 25  
Poisson's Ratio 0.27-0.30 25  
Elastic Modulus (GPa) 190-210 25  
Tensile Strength (Mpa) 640  25  cold drawn, spheroidized annealed  more
Yield Strength (Mpa) 495 
Elongation (%) 10 
Reduction in Area (%) 45 
Hardness (HB) 192  25  cold drawn, spheroidized annealed more

Thermal Properties
Properties Conditions 
T (°C)Treatment
Thermal Expansion (10-6/ºC) 11.8  0-100 more rolled 