AISI 1137 |
 |
|
| Category | Steel |
| Class | Carbon steel |
| Type | Standard resulfurized |
| Designations |
United States: AMS 5020 , AMS 5024C , AMS 5024D , ASTM A108 , ASTM A29 , ASTM A311 , FED QQ-S-637 (1137) , SAE J403 , SAE J412 , SAE J414 , UNS G11370
|
| Composition |
 |
|
| Element | Weight % |
| C |
0.32-0.39 |
| Mn |
1.35-1.65 |
| P |
0.04 (max) |
| S |
0.08-0.13 |
|
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
7.7-8.03
|
25 |
|
| Poisson's Ratio |
0.27-0.30 |
25 |
|
| Elastic Modulus (GPa) |
190-210
|
25 |
|
| Tensile Strength (Mpa) |
584.7 |
25 |
annealed at 790°C more |
| Yield Strength (Mpa) |
344.7 |
| Elongation (%) |
26.8 |
| Reduction in Area (%) |
53.9 |
| Hardness (HB) |
174 |
25 |
annealed at 790°C more |
Impact Strength (J) (Izod) |
49.9 |
25 |
annealed at 790°C more |
|