UNS C82700 |
 |
|
| Category | Copper Alloy |
| Class | Cast |
| Type | High-copper alloy |
| Designations | United States: UNS C82700 |
| Composition |
 |
|
| Element | Weight % |
| Cu |
96.3 |
| Be |
2.45 |
| Ni |
1.25 |
|
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
8.8-8.94
|
25 |
|
| Poisson's Ratio |
0.34 |
25 |
|
| Elastic Modulus (GPa) |
117
|
25 |
|
| Tensile Strength (Mpa) |
(1069) |
25 |
(castings: centrifugal, investment, permanent mold, plaster, sand) |
| Yield Strength (Mpa) |
(896) |
| Elongation (%) |
(0) |
| Reduction in Area (%) |
|
| Note: Values in parentheses indicate responses to heat treatment |
| Hardness (HRC) |
(39) |
25 |
(as cast) |
| Note: Value in parentheses indicates response to heat treatment. |
|