ASTM AZ63A-T6 |
 |
|
| Category | Magnesium Alloy |
| Designations | United States: UNS S24100, ASTM A276, ASTM A580 |
| Composition |
 |
|
| Element | Weight % |
| Al |
6.00 |
| Mn |
0.15 |
| Zn |
3.00 |
|
|
| Mechanical Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Density (×1000 kg/m3) |
1.84 |
25 |
|
| Poisson's Ratio |
0.35 |
25 |
|
| Elastic Modulus (GPa) |
44.8
|
25 |
|
| Tensile Strength (Mpa) |
275.0 |
25 |
T6 (sand casting, permanent mold casting) |
| Yield Strength (Mpa) |
130.0 |
| Elongation (%) |
5.0 |
| Reduction in Area (%) |
|
| Hardness (HB500) |
73 |
25 |
T6 (sand casting, permanent mold casting) |
| Shear Strength (MPa) |
145 |
25 |
T6 (sand casting, permanent mold casting) |
| Thermal Properties |
 |
|
| Properties | Conditions |
| T (°C) | Treatment |
| Thermal Expansion (10-6/ºC) |
26.1 |
20-100 |
T6 |
| Thermal Conductivity (W/m-K) |
75.3 |
0 |
T6 |
|