Thermal Conductivity: Silver
engineering fundamentals Thermal Conductivity: Silver
Directory | Career | News | Industrial
Home Membership Magazines Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Silver
 
Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 3940
2 101325 7830
3 101325 11500
4 101325 14700
5 101325 17200
6 101325 18700
7 101325 19300
8 101325 19000
9 101325 18100
10 101325 16800
15 101325 9600
20 101325 5110
30 101325 1930
40 101325 1050
50 101325 700
60 101325 550
70 101325 497
80 101325 471
90 101325 460
100 101325 450
150 101325 432
200 101325 430
250 101325 429
300 101325 429
350 101325 427
400 101325 425
500 101325 419
600 101325 412
800 101325 396
1000 101325 379
1200 101325 361