Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 546
2 101325 1090
3 101325 1610
4 101325 2090
5 101325 2520
6 101325 2850
7 101325 3090
8 101325 3230
9 101325 3270
10 101325 3240
15 101325 2460
20 101325 1580
30 101325 755
40 101325 515
50 101325 421
60 101325 374
70 101325 348
80 101325 332
90 101325 328
100 101325 327
150 101325 325
200 101325 323
250 101325 321
300 101325 317
350 101325 314
400 101325 311
500 101325 304
600 101325 298
800 101325 284
1000 101325 270
1200 101325 255