Thermal Conductivity: Chromium
engineering fundamentals Thermal Conductivity: Chromium
Directory | Career | News | Industrial
Home Membership Magazines Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Chromium
 
Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 40.2
2 101325 80.3
3 101325 120
4 101325 160
5 101325 200
6 101325 239
7 101325 227
8 101325 314
9 101325 350
10 101325 385
15 101325 524
20 101325 593
30 101325 549
40 101325 425
50 101325 317
60 101325 248
70 101325 207
80 101325 184
90 101325 169
100 101325 159
150 101325 129
200 101325 111
250 101325 100
300 101325 93.7
350 101325 92.9
400 101325 90.9
500 101325 86
600 101325 80.7
800 101325 71.3
1000 101325 65.4
1200 101325 61.9
1400 101325 58.8
1600 101325 55.6
1800 101325 52.6
2000 101325 49.4