Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 171
2 101325 342
3 101325 511
4 101325 677
5 101325 839
6 101325 993
7 101325 1140
8 101325 1270
9 101325 1390
10 101325 1480
15 101325 1700
20 101325 1540
30 101325 1000
40 101325 623
50 101325 405
60 101325 285
70 101325 216
80 101325 175
90 101325 150
100 101325 134
150 101325 104
200 101325 94
250 101325 86.5
300 101325 80.2
350 101325 74.4
400 101325 69.5
500 101325 61.3
600 101325 54.7
800 101325 43.3
1000 101325 32.3
1200 101325 28.3
1400 101325 31.2
1600 101325 33
1800 101325 34.5