Thermal Conductivity: Germanium
engineering fundamentals Thermal Conductivity: Germanium
Directory | Career | News | Standards | Industrial | SpecSearch®
Home Membership Magazines Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Germanium
 
Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 27.4
2 101325 206
3 101325 535
4 101325 877
5 101325 1160
6 101325 1390
7 101325 1550
8 101325 1660
9 101325 1730
10 101325 1770
15 101325 1730
20 101325 1490
30 101325 1080
40 101325 798
50 101325 615
60 101325 487
70 101325 393
80 101325 325
90 101325 270
100 101325 232
150 101325 132
200 101325 96.8
250 101325 74.9
300 101325 59.9
350 101325 49.5
400 101325 43.2
500 101325 33.8
600 101325 27.3
800 101325 19.8
1000 101325 17.4
1200 101325 17.4
Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2018 eFunda, Inc.