Thermal Conductivity: Nickel
engineering fundamentals Thermal Conductivity: Nickel
Directory | Career | News | Standards | Industrial | SpecSearch®
Home Membership Magazines Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Nickel
 
Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 217
2 101325 434
3 101325 649
4 101325 859
5 101325 1060
6 101325 1250
7 101325 1420
8 101325 1580
9 101325 1710
10 101325 1810
15 101325 1950
20 101325 1650
30 101325 956
40 101325 582
50 101325 400
60 101325 308
70 101325 250
80 101325 210
90 101325 183
100 101325 164
150 101325 122
200 101325 107
250 101325 97.5
300 101325 90.7
350 101325 85
400 101325 80.2
500 101325 72.2
600 101325 65.6
800 101325 67.6
1000 101325 71.8
1200 101325 76.2
1400 101325 80.4