Lead
 
Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 2790
2 101325 4460
3 101325 3580
4 101325 2220
5 101325 1380
6 101325 810
7 101325 486
8 101325 320
9 101325 230
10 101325 178
15 101325 84.5
20 101325 59.1
30 101325 47.7
40 101325 45.1
50 101325 43.6
60 101325 42.5
70 101325 41.6
80 101325 40.9
90 101325 40.3
100 101325 39.7
150 101325 37.9
200 101325 36.7
250 101325 36
300 101325 35.3
350 101325 34.7
400 101325 34
500 101325 32.8
600 101325 31.4