Platinum
 
Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 231
2 101325 460
3 101325 679
4 101325 880
5 101325 1050
6 101325 1180
7 101325 1260
8 101325 1290
9 101325 1280
10 101325 1230
15 101325 841
20 101325 495
30 101325 215
40 101325 139
50 101325 109
60 101325 94.7
70 101325 86.2
80 101325 81.5
90 101325 78.9
100 101325 77.5
150 101325 74
200 101325 72.6
250 101325 71.8
300 101325 71.6
350 101325 71.7
400 101325 71.8
500 101325 72.3
600 101325 73.2
800 101325 75.6
1000 101325 78.7
1200 101325 82.6
1400 101325 87.1
1600 101325 91.9
1800 101325 96.1
2000 101325 99.4