Thermal Conductivity: Silicon
engineering fundamentals Thermal Conductivity: Silicon
Directory | Career | News | Standards | Industrial | SpecSearch®
Home Membership Magazines Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Silicon
 
Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 6.93
2 101325 45.4
3 101325 138
4 101325 297
5 101325 527
6 101325 823
7 101325 1170
8 101325 1550
9 101325 1950
10 101325 2330
15 101325 4160
20 101325 4980
30 101325 4810
40 101325 3530
50 101325 2680
60 101325 2110
70 101325 1680
80 101325 1340
90 101325 1080
100 101325 884
150 101325 409
200 101325 264
250 101325 191
300 101325 148
350 101325 119
400 101325 98.9
500 101325 76.2
600 101325 61.9
800 101325 42.2
1000 101325 31.2
1200 101325 25.7
1400 101325 23.5
1600 101325 22.1