Tin
 
Conditions Thermal Conductivity (W/m-K)
Temperature (K) Pressure (Pa)
1 101325 18300
2 101325 32300
3 101325 29700
4 101325 18100
5 101325 11700
6 101325 7600
7 101325 5200
8 101325 3600
9 101325 2600
10 101325 1930
15 101325 630
20 101325 320
30 101325 179
40 101325 133
50 101325 115
60 101325 104
70 101325 96
80 101325 91.5
90 101325 88
100 101325 85.3
150 101325 77.9
200 101325 73.3
250 101325 69.6
300 101325 66.6
350 101325 64.2
400 101325 62.2
500 101325 59.6