eFunda Polymers: Properties of ABS {ABS / Nylon}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
ABS
 
List of Suppliers
Additives: ABS / Nylon
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   1794 - 2208  tensile   D638
Flexural Modulus (MPa)   1725 - 2139   23 ºC   D790
Tensile Strength (MPa)   28 - 42 at break   D638
  30 - 44 at yield   D638
Flexural Strength (MPa)
at yield or break
  61 - 76     D790
Elongation at break (%)   40 - 300     D638
Hardness   93 - 105  Rockwell R   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  8.0 - 10.6     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   90 - 110     D696
Deflection Temperature (ºC)   83 - 91   0.46 MPa   D648
  55 - 66   1.82 MPa   D648

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.06 - 1.07   D792

 Processing Properties Conditions
Type ASTM
Processing Temperature (ºC)  238 - 272  injection molding  
Molding Pressure (MPa)   56 - 173    
Compression Ratio  1.1 - 2    
Linear Mold Shrinkage (cm/cm)  0.003 - 0.01   D955