eFunda Polymers: Properties of Fluoroplastics {PTFE, 25% glass fiber reinforced}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Fluoroplastics
 
List of Suppliers
State: PTFE
Additives: 25% glass fiber reinforced
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   1380 - 1656  tensile   D638
Flexural Modulus (MPa)   1311 - 1622   23 ºC   D790
Tensile Strength (MPa)   14 - 19 at break   D638
Compressive Strength (MPa)
at yield or break
  7 - 10  at 1% strain   D695
Flexural Strength (MPa)
at yield or break
  14     D790
Elongation at break (%)   200 - 300     D638
Hardness   60 - 70  Shore D   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  1.4     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   77 - 100     D696
Thermal Conductivity (W/m-ºC)  0.334 - 0.418     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  2.2 - 2.3   D792
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  320   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  327  Tm, crystalline  
Molding Pressure (MPa)   21 - 56    
Linear Mold Shrinkage (cm/cm)  0.018 - 0.02   D955

Top of Page

Suppliers
Ausimont USA, Inc. Thorofare, NJ  800-323-2874
DuPont Co., Polymers Wilmington, DE  800-438-7225
Dyneon Oakdale, MN  800-863-9374
ICI Americas, Inc. Wilmington, DE   
RTP Co. Winona, MN  800-433-4787

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.