eFunda Polymers: Properties of Polyamide {nylon (PA 66), 40% glass and mineral reinforced}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyamide
 
List of Suppliers
State: nylon (PA 66)
Additives: 40% glass and mineral reinforced
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Flexural Modulus (MPa)   6797 - 12075   23 ºC  dry (0.2% water content) D790
  4140   23 ºC  50% relative humidity D790
  4140   94 ºC   D790
Tensile Strength (MPa)  107 - 214 at break  dry (0.2% water content) D638
  91 at break  50% relative humidity D638
Compressive Strength (MPa)
at yield or break
 125 - 256  dry (0.2% water content)   D695
Flexural Strength (MPa)
at yield or break
 166 - 332  dry (0.2% water content)   D790
Elongation at break (%)   2 - 7    dry (0.2% water content) D638
Hardness   95 - 98  Rockwell M  dry (0.2% water content) D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.3 - 2.0    dry (0.2% water content) D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   20 - 54     D696
Deflection Temperature (ºC)  249 - 258   0.46 MPa  dry (0.2% water content) D648
 223 - 252   1.82 MPa  dry (0.2% water content) D648
Thermal Conductivity (W/m-ºC)  0.460     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.42 - 1.55   D792
Water Absorption (% weight increase)  5.1  saturated D570
 0.4 - 0.9  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  300 - 525   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  250 - 260  Tm, crystalline  
Processing Temperature (ºC)  266 - 310  injection molding  
Molding Pressure (MPa)   63 - 138    
Compression Ratio  3 - 4    
Linear Mold Shrinkage (cm/cm)  0.001 - 0.005   D955

Top of Page

Suppliers
Adell Plastics, Inc. Baltimore, MD  800-638-5218
ALM Corp. Wayne, NJ   
Ashley Polymers Brooklyn, NY   
BASF Corp. Mount Olive, NJ  800-BC-RESIN
ComAlloy International Co. Nashville, TN   
DSM Engineering Plastic Products, Inc. Reading, PA  800-729-0101
DuPont Co., Polymers Wilmington, DE  800-438-7225
EMS-American Grilon, Inc. Sumter, SC   
Ferro Corp. Cleveland, OH   
LNP Engineering Plastics, Inc. Exton, PA  800-854-8774
M.A. Hanna Engineered Materials Norcross, GA   
MRC Polymers, Inc. Chicago, IL   
Network Polymers, Inc. Akron, OH  888-437-4674
Nyltech NA Co., Inc. Manchester, NH   
RTP Co. Winona, MN  800-433-4787
Solutia, Inc. St Louis, MO   
Thermofil, Inc. Brighton, MI  800-444-4408
Ticona Summit, NJ  800-526-4960
Wellman, Inc. Johnsonville, SC   

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.