eFunda Polymers: Properties of Polyamide {nylon (PA 66), 30% pitch carbon fiber, EMI shielding (conductive)}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyamide
 
List of Suppliers
State: nylon (PA 66)
Additives: 30% pitch carbon fiber
Application: EMI shielding (conductive)
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   9660 - 13800  tensile  dry (0.2% water content) D638
Flexural Modulus (MPa)   8280 - 10350   23 ºC  dry (0.2% water content) D790
Tensile Strength (MPa)  107 - 108 at break  dry (0.2% water content) D638
Compressive Strength (MPa)
at yield or break
 142     D695
Flexural Strength (MPa)
at yield or break
 172 - 180  dry (0.2% water content)   D790
Elongation at break (%)   2    dry (0.2% water content) D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.3 - 0.4    dry (0.2% water content) D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   16 - 19     D696
Deflection Temperature (ºC)  255 - 260   0.46 MPa   D648
 241 - 255   1.82 MPa   D648

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.3 - 1.31   D792
Water Absorption (% weight increase)  0.6  after 24 hrs D570

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  260 - 265  Tm, crystalline  
Processing Temperature (ºC)  277 - 299  injection molding  
Linear Mold Shrinkage (cm/cm)  0.003   D955

Top of Page

Suppliers
ComAlloy International Co. Nashville, TN   
LNP Engineering Plastics, Inc. Exton, PA  800-854-8774
Polymers International, Inc. Spartanburg, SC   
RTP Co. Winona, MN  800-433-4787