eFunda Polymers: Properties of Polyethylene and ethylene copolymers {crosslinked, molding grade}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polyethylene and ethylene copolymers
 
List of Suppliers
State: crosslinked
Application: molding grade
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   345 - 3450  tensile   D638
  345 - 1035  compressive   D638
Flexural Modulus (MPa)   483 - 2415   23 ºC   D790
Tensile Strength (MPa)   12 - 32 at break   D638
Compressive Strength (MPa)
at yield or break
  14 - 38     D695
Flexural Strength (MPa)
at yield or break
  14 - 45     D790
Elongation at break (%)   10 - 440     D638
Hardness   55 - 80  Shore D   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.5 - 10.6     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)  100     D696
Deflection Temperature (ºC)   55 - 108   0.46 MPa   D648
  41 - 63   1.82 MPa   D648

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  0.95 - 1.45   D792
Water Absorption (% weight increase)  0.01 - 0.06  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  230 - 550   D149

 Processing Properties Conditions
Type ASTM
Processing Temperature (ºC)  116 - 233  compression molding  
 122 - 149  injection molding  
Linear Mold Shrinkage (cm/cm)  0.007 - 0.09   D955

Top of Page

Suppliers
A. Schulman Akron, OH  800-662-7203
Equistar Chemicals LP Houston, TX  888-777-0232
Mobil Chemical Co. Edison, NJ   
Phillips Chemical Co. Bartlesville, OK  800-537-3746

Top of Page