eFunda Polymers: Properties of Polystyrene and styrene copolymers {styrene / acrylonitrile, copolymer, molding and extrusion}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Polystyrene and styrene copolymers
 
List of Suppliers
State: styrene / acrylonitrile, copolymer
Application: molding and extrusion
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   3657 - 4002  compressive   D638
  3278 - 3864  tensile   D638
Flexural Modulus (MPa)   3450 - 4209   23 ºC   D790
Tensile Strength (MPa)   69 - 83 at break   D638
  69 - 83 at yield   D638
Compressive Strength (MPa)
at yield or break
  97 - 104     D695
Flexural Strength (MPa)
at yield or break
  76 - 132     D790
Elongation at break (%)   2 - 3     D638
Hardness   83 - 75  Rockwell R   D638
  80  Rockwell M   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.2 - 0.3     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   65 - 68     D696
Deflection Temperature (ºC)  105 - 107   0.46 MPa   D648
  95 - 105   1.82 MPa   D648
Thermal Conductivity (W/m-ºC)  0.125     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.06 - 1.08   D792
Water Absorption (% weight increase)  0.5  saturated D570
 0.15 - 0.25  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  425   D149

 Processing Properties Conditions
Type ASTM
Melt Flow (gm/10 min)  1.4   D1238
Melting Temperature (ºC)  100 - 200  Tg, amorphous  
Processing Temperature (ºC)  149 - 205  compression molding  
 183 - 288  injection molding  
 183 - 233  extrusion  
Molding Pressure (MPa)   35 - 138    
Compression Ratio  3    
Linear Mold Shrinkage (cm/cm)  0.003 - 0.005   D955

Top of Page

Suppliers
A. Schulman Akron, OH  800-662-7203
Albis Corp. Rosenburg, TX  800-231-5911
American Polymers, Inc. Worcester, MA   
Bamberger Polymers, Inc. Jericho, NY   
BASF Corp. Mount Olive, NJ  800-BC-RESIN
Bayer Corp. Pittsburgh, PA  800-662-2927
Dow Plastics Midland, MI  800-441-4369
Federal Plastics Corp. Cranford, NJ  800-541-4424
Huntsman Corp. Salt Lake City, UT  800-421-2411
LG Chemical America, Inc. Englewood Cliffs, NJ   
Network Polymers, Inc. Akron, OH  888-437-4674
R.S.G. Polymers Corp. Stony Brook, NY   

Top of Page