eFunda Polymers: Properties of Vinyl polymers and copolymers {PVC and PVC-AMC, sheets, rods and tubes; rigid}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Vinyl polymers and copolymers
 
List of Suppliers
State: PVC and PVC-AMC
Application: sheets, rods and tubes; rigid
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   2415 - 4140  tensile   D638
Flexural Modulus (MPa)   2070 - 3450   23 ºC   D790
Tensile Strength (MPa)   41 - 52 at break   D638
  41 - 45 at yield   D638
Compressive Strength (MPa)
at yield or break
  56 - 90     D695
Flexural Strength (MPa)
at yield or break
  69 - 111     D790
Elongation at break (%)   40 - 80     D638
Hardness   65 - 85  Shore D   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.2 - 11.7     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   50 - 100     D696
Deflection Temperature (ºC)   58 - 83   0.46 MPa   D648
  60 - 77   1.82 MPa   D648
Thermal Conductivity (W/m-ºC)  0.146 - 0.209     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.3 - 1.58   D792
Water Absorption (% weight increase)  0.04 - 0.4  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  350 - 500   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)   75 - 105  Tg, amorphous  
Processing Temperature (ºC)  141 - 205  compression molding  
 149 - 213  injection molding  
Molding Pressure (MPa)   69 - 276    
Compression Ratio  2 - 2.3    
Linear Mold Shrinkage (cm/cm)  0.002 - 0.006   D955

Top of Page

Suppliers
AlphaGary Corp. Leominster, MA  800-232-9741
Colorite Plastic Co. Ridgefield, NJ  800-631-1577
CONDEA Vista Co. Houston, TX  800-841-4877
Creanova, Inc. Somerset, NJ   
Formosa Plastics Corp. Livingston, NJ  888-372-8723
Georgia Gulf Corp. Atlanta, GA   
Keysor-Century Corp. Santa Clarita, CA  888-539-7671
LG Chemical America, Inc. Englewood Cliffs, NJ   
Novatec Plastics & Chemicals Co., Inc. Eatontown, NJ  800-782-6682
Occidental Chemical Corp. Dallas, TX  800-578-8880
R.S.G. Polymers Corp. Stony Brook, NY   
Rimtec Corp. Burlington, NJ  800-272-0069
Shintech Inc. Houston, TX   
Synergistic Polymer Systems, Inc. Bellaire, TX   
Union Carbide Corp. Danbury, CT  800-335-8550
Vi-Chem Corp. Grand Rapids, MI  800-477-8501