eFunda Polymers: Properties of Thermoplastic elastomers {polyether/amide block copolymer}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Thermoplastic elastomers
 
List of Suppliers
State: polyether/amide block copolymer
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   14 - 414  tensile   D638
Flexural Modulus (MPa)   21 - 456   23 ºC   D790
Tensile Strength (MPa)   14 - 49 at break   D638
  21 - 25 at yield   D638
Flexural Strength (MPa)
at yield or break
  8 - 14     D790
Elongation at break (%)   350 - 680     D638
Hardness   75  Shore A   D638
  72  Shore D   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  2.3 - 0     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)  210 - 230     D696
Deflection Temperature (ºC)   70 - 125   0.46 MPa   D648
  8 - 58   1.82 MPa   D648

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1 - 1.03   D792
Water Absorption (% weight increase)  1.01 - 1.36  after 24 hrs D570

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  148 - 209  Tm, crystalline  
Processing Temperature (ºC)  185 - 249  compression molding  
 172 - 250  injection molding  
 172 - 238  extrusion  
Molding Pressure (MPa)   56 - 83    

Top of Page

Suppliers
Creanova, Inc. Somerset, NJ   
Elf Atochem North America, Inc. Philadelphia, PA  800-225-7788