eFunda Polymers: Properties of Acrylic {poly(methylmethacrylate), PMMA, molding and extrusion compounds}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Acrylic
 
List of Suppliers
State: poly(methylmethacrylate), PMMA
Application: molding and extrusion compounds
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   2553 - 3174  compressive   D638
  2243 - 3243  tensile   D638
Flexural Modulus (MPa)   2243 - 3174   23 ºC   D790
Tensile Strength (MPa)   49 - 73 at break   D638
  54 - 74 at yield   D638
Compressive Strength (MPa)
at yield or break
  73 - 125     D695
Flexural Strength (MPa)
at yield or break
  73 - 132     D790
Elongation at break (%)   2 - 6     D638
Hardness   68 - 105  Rockwell M   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.1 - 0.2     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   50 - 90     D696
Deflection Temperature (ºC)   74 - 108   0.46 MPa   D648
  69 - 100   1.82 MPa   D648
Thermal Conductivity (W/m-ºC)  0.167 - 0.251     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.17 - 1.2   D792
Water Absorption (% weight increase)  0.1 - 0.4  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  400 - 500   D149

 Processing Properties Conditions
Type ASTM
Melt Flow (gm/10 min)  1.4 - 27   D1238
Melting Temperature (ºC)   85 - 105  Tg, amorphous  
Processing Temperature (ºC)  163 - 260  injection molding  
 183 - 260  extrusion  
 149 - 219  compression molding  
Molding Pressure (MPa)   35 - 138    
Compression Ratio  1.6 - 3    
Linear Mold Shrinkage (cm/cm)  0.001 - 0.004  flow direction D955
Linear Mold Shrinkage (cm/cm)  0.002 - 0.008  transverse dir. D955

Top of Page

Suppliers
American Polymers, Inc. Worcester, MA   
AtoHaas Americas, Inc. Philadelphia, PA   
Continental Acrylics, Inc. Compton, CA  800-562-8883
Cyro Industries Rockaway, NJ  800-631-5384
DuPont Co., Polymers Wilmington, DE  800-438-7225
ICI Acrylics, Inc. Cordova, TN  800-325-9577
LG Chemical America, Inc. Englewood Cliffs, NJ   
Network Polymers, Inc. Akron, OH  888-437-4674
Plaskolite, Inc. Columbus, OH  800-848-9124
RTP Co. Winona, MN  800-433-4787

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.