eFunda Polymers: Properties of Epoxy {flexibilized, casting resins and compounds}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Epoxy
 
List of Suppliers
Additives: flexibilized
Application: casting resins and compounds
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)   7 - 2415  compressive   D638
Tensile Strength (MPa)   14 - 69 at break   D638
Compressive Strength (MPa)
at yield or break
  7 - 97     D695
Flexural Strength (MPa)
at yield or break
  7 - 90     D790
Elongation at break (%)   20 - 85     D638
Hardness   65 - 89  Shore D   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  1.2 - 2.7     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   20 - 100     D696
Deflection Temperature (ºC)   23 - 122   1.82 MPa   D648

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  0.96 - 1.35   D792
Water Absorption (% weight increase)  0.27 - 0.5  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  235 - 400   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  thermoset  Tm, crystalline  
Linear Mold Shrinkage (cm/cm)  0.001 - 0.01   D955

Top of Page

Suppliers
Conap, Inc. Olean, NY  800-836-3666
Dow Plastics Midland, MI  800-441-4369
Emerson & Cuming Specialty Polymers Billerica, MA  800-832-4929
Epic Resins Palmyra, WI  800-242-6649
ITW Devcon Danvers, MA  800-933-8266

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.