eFunda Polymers: Properties of Phenolic {phenol-formaldehyde, high strength glass fiber reinforced, molding compounds}
engineering fundamentals Polymer Material Properties
Directory | Career | News | Standards | Industrial | SpecSearch®
Generic (ABS, ...) Trade Name
Materials Home
General Information
Polymer Home
Glossary
Material Science
Overview
Characteristics
Comparisons
Selection Criteria
Applications
Flow Characteristics
Datasheet Primer
Major Categories
Polymer Index
History Timeline
List by Process
List by ThermoP/S
Specific Polymer
Category / Grades
Datasheet
Supplier Info
Resources
Bibliography


Login

Home Membership Store Forum Search Member Calculators

Materials

Design

Processes

Units

Formulas

Math
 
Phenolic
 
List of Suppliers
State: phenol-formaldehyde
Additives: high strength glass fiber reinforced
Application: molding compounds
Material Properties
 Mechanical Properties Conditions
State 1 State 2 ASTM
Elastic Modulus (MPa)  13110 - 22770  tensile   D638
 18906 - 24150  compressive   D638
Flexural Modulus (MPa)   7935 - 22770   23 ºC   D790
Tensile Strength (MPa)   49 - 125 at break   D638
Compressive Strength (MPa)
at yield or break
 111 - 483     D695
Flexural Strength (MPa)
at yield or break
  83 - 414     D790
Elongation at break (%)   1     D638
Hardness   54 - 101  Rockwell E   D638
  72  Barcol   D638
Izod Impact (J/cm of notch)
1/8" thick specimen unless noted
  0.3 - 9.5     D256A

 Thermal Properties Conditions
Pressure State ASTM
Coef of Thermal Expansion (10-6/ºC)   8 - 34     D696
Deflection Temperature (ºC)  177 - 316   1.82 MPa   D648
Thermal Conductivity (W/m-ºC)  0.334 - 0.585     C177

 Physical & Electrical Properties Conditions
State ASTM
Specific Gravity  1.69 - 2   D792
Water Absorption (% weight increase)  0.12 - 1.5  saturated D570
 0.03 - 1.2  after 24 hrs D570
Dielectric Strength (V/mil);
1/8" thick specimen unless noted
  140 - 400   D149

 Processing Properties Conditions
Type ASTM
Melting Temperature (ºC)  thermoset  Tm, crystalline  
Processing Temperature (ºC)  149 - 194  compression molding  
 149 - 177  transfer molding  
 166 - 199  injection molding  
Molding Pressure (MPa)   7 - 138    
Compression Ratio  2 - 10    
Linear Mold Shrinkage (cm/cm)  0.001 - 0.004   D955

Top of Page

Suppliers
Cytec Fiberite, Inc. Tempe, AZ   
Occidental Chemical Corp. Dallas, TX  800-578-8880
Plastics Engineering, Inc. Auburn Hills, MI   
Quantum Composites, Inc. Midland, MI  800-462-9318
Resinoid Engineering Corp. Hebron, OH   
Rogers Corp. Rogers, CT  800-227-6437

Top of Page

Home  Membership  About Us  Privacy  Disclaimer  Contact  Advertise

Copyright © 2009 eFunda, Inc.